Komposisi kimia
Kelas | C | MN | Si | P | S | CR |
15KCuBNb5-6-4 | ≤0.17 | 0.8-1.2 | 0.25-0.50 | ≤0.03 | ≤0.025 | ≤0.30 |
CU | MO | NI | Jml | N | ||
0.5-0.8 | 0.25-0.50 | 1.00-1.30 | 0.015-0.045 | ≤0.02 |
Kelas | Kekuatan yield/MPa | Kekuatan tensil/Mpa | Naskh/% | Kekerasan/HB | Berdampak pada longitudinal/J pekerjaan | Microstruktur | ||
20 DERAJAT CELCIUS | CELCIUS | -20 DERAJAT | ||||||
15KCuBNb5-6-4 | ≥440 | 610-780 | ≥19 | ≤252 | ≥95 | ≥80 | ≥60 | F+B+P |
Kelas | 400 | 420C | 440 | 460 DERAJAT CELCIUS | 480C | 490 | 500 DERAJAT |
15KCuBNb5-6-4 | 373 | 325 | 273 | 210 | 139 | 104 | 69 |
Normalizing atau penikalan | Mengeraskan | Perawatan dengan bebas stres |
900-980 Applying air | 580-640 Applying air | 550-600 Applying air |
880-930 terwujudnya cairan pendingin air dan minyak | 620-700 Applying air |